T 80 K (-193 °C) 273 K (0 °C) 293 K (20 °C) 298 K (25 °C) 300 K (27 °C) 500 K (227 °C)
3 Li lithium
use 10.0 n?m 85.3 n?m 92.8 n?m 94.7 n?m 95.5 n?m
CRC (10-8 ?m) 1.00 8.53 9.28 9.47 9.55
LNG (10-8 ?m) 9.28
WEL (10-8 ?m) (293 K-298 K) 9.4
4 Be beryllium
use 0.75 n?m 30.2 n?m 35.6 n?m 37.0 n?m 37.6 n?m 99 n?m
CRC (10-8 ?m) 0.075 3.02 3.56 3.70 3.76 9.9
LNG (10-8 ?m) 3.56
WEL (10-8 ?m) (293 K-298 K) 4
5 B boron
use 1.5×104 ?m
LNG (10-8 ?m) 1.5×1012
WEL (10-8 ?m) (293 K-298 K) > 1012
6 C carbon (diamond)
use
LNG (10-8 ?m) 0.8 [sic]
6 C carbon (graphite)
use
LNG (10-8 ?m) 1375
WEL (10-8 ?m) (293 K-298 K) about 1000 - direction dependent
11 Na sodium
use 8.0 n?m 43.3 n?m 47.7 n?m 48.8 n?m 49.3 n?m
CRC (10-8 ?m) 0.80 4.33 4.77 4.88 4.93
LNG (10-8 ?m) 4.77
WEL (10-8 ?m) (293 K-298 K) 4.7
12 Mg magnesium
use 5.57 n?m 40.5 n?m 43.9 n?m 44.8 n?m 45.1 n?m 78.6 n?m
CRC (10-8 ?m) 0.557 4.05 4.39 4.48 4.51 7.86
LNG (10-8 ?m) 4.39
WEL (10-8 ?m) (293 K-298 K) 4.4
13 Al aluminium
use 2.45 n?m 24.17 n?m 26.50 n?m 27.09 n?m 27.33 n?m 49.9 n?m
CRC (10-8 ?m) 0.245 2.417 2.650 2.709 2.733 4.99
LNG (10-8 ?m) 2.6548
WEL (10-8 ?m) (293 K-298 K) 2.65
14 Si silicon
use
LNG (10-8 ?m) 105
WEL (10-8 ?m) (293 K-298 K) about 100000
15 P phosphorus
use
LNG (10-8 ?m) (white) 10 [sic]
WEL (10-8 ?m) (293 K-298 K) 10
16 S sulfur
use (amorphous) 2×1015 ?m
LNG (10-8 ?m) (amorphous) 2×1023
WEL (10-8 ?m) (293 K-298 K) > 1023
17 Cl chlorine
use > 10 ?m
LNG (10-8 ?m) >109
WEL (10-8 ?m) (293 K-298 K) > 1010
19 K potassium
use 13.4 n?m 64.9 n?m 72.0 n?m 73.9 n?m 74.7 n?m
CRC (10-8 ?m) 1.34 6.49 7.20 7.39 7.47
LNG (10-8 ?m) 7.2
WEL (10-8 ?m) (293 K-298 K) 7
20 Ca calcium
use 6.5 n?m 31.1 n?m 33.6 n?m 34.2 n?m 34.5 n?m 60. n?m
CRC (10-8 ?m) 0.65 3.11 3.36 3.42 3.45 6.0
LNG (10-8 ?m) 3.36
WEL (10-8 ?m) (293 K-298 K) 3.4
21 Sc scandium
use (room temperature) (alpha, polycrystalline) calculated 562 n?m
CRC (10-8 ?m) (290 K-300 K) 56.2
CR2 (10-8 ?m) (room temperature) (alpha, amorphous) 70.9
CR2 (10-8 ?m) (room temperature) (alpha, crystalline) 26.9
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) calculated from single crystal values 56.2
LNG (10-8 ?m) 56.2
WEL (10-8 ?m) (293 K-298 K) 55
22 Ti titanium
use 0.39 µ?m 0.420 µ?m
CRC (10-8 ?m) 39
LNG (10-8 ?m) 42.0
WEL (10-8 ?m) (293 K-298 K) 40
23 V vanadium
use 24.1 n?m 181 n?m 197 n?m 201 n?m 202 n?m 348 n?m
CRC (10-8 ?m) 2.41 18.1 19.7 20.1 20.2 34.8
LNG (10-8 ?m) 19.7
WEL (10-8 ?m) (293 K-298 K) 20
24 Cr chromium
use 118 n?m 125 n?m 126 n?m 127 n?m 201 n?m
CRC (10-8 ?m) 11.8 12.5 12.6 12.7 20.1
LNG (10-8 ?m) 12.5
WEL (10-8 ?m) (293 K-298 K) 12.7
25 Mn manganese
use 1.32 µ?m 1.43 µ?m 1.44 µ?m 1.44 µ?m 1.44 µ?m 1.49 µ?m
CRC (10-8 ?m) 132 143 144 144 144 149
LNG (10-8 ?m) 144
WEL (10-8 ?m) (293 K-298 K) 160
26 Fe iron
use 6.93 n?m 85.7 n?m 96.1 n?m 98.7 n?m 99.8 n?m 237 n?m
CRC (10-8 ?m) 0.693 8.57 9.61 9.87 9.98 23.7
LNG (10-8 ?m) 9.61
WEL (10-8 ?m) (293 K-298 K) 9.7
27 Co cobalt
use 56 n?m 62.4 n?m
CRC (10-8 ?m) 5.6
LNG (10-8 ?m) 6.24
WEL (10-8 ?m) (293 K-298 K) 6
28 Ni nickel
use 5.45 n?m 61.6 n?m 69.3 n?m 71.2 n?m 72.0 n?m 177 n?m
CRC (10-8 ?m) 0.545 6.16 6.93 7.12 7.20 17.7
LNG (10-8 ?m) 6.93
WEL (10-8 ?m) (293 K-298 K) 7
29 Cu copper
use 2.15 n?m 15.43 n?m 16.78 n?m 17.12 n?m 17.25 n?m 30.90 n?m
CRC (10-8 ?m) 0.215 1.543 1.678 1.712 1.725 3.090
LNG (10-8 ?m) 1.678
WEL (10-8 ?m) (293 K-298 K) 1.7
30 Zn zinc
use 11.5 n?m 54.6 n?m 59.0 n?m 60.1 n?m 60.6 n?m 108.2 n?m
CRC (10-8 ?m) 1.15 5.46 5.90 6.01 6.06 10.82
LNG (10-8 ?m) 5.9
WEL (10-8 ?m) (293 K-298 K) 5.9
31 Ga gallium
use
CRC (10-8 ?m) 13.6
LNG (10-8 ?m) (30 °C) 25.795
WEL (10-8 ?m) (293 K-298 K) 14
32 Ge germanium
use
LNG (10-8 ?m) 53000
WEL (10-8 ?m) (293 K-298 K) about 50000
33 As arsenic
use 333 n?m
LNG (10-8 ?m) 33.3
WEL (10-8 ?m) (293 K-298 K) 30
34 Se selenium
use
LNG (10-8 ?m) (amorphous) 1.2 [sic]
WEL (10-8 ?m) (293 K-298 K) high
35 Br bromine
use 7.8×1010 ?m
LNG (10-8 ?m) 7.8×1018
WEL (10-8 ?m) (293 K-298 K) > 1018
37 Rb rubidium
use 26.5 n?m 115 n?m 128 n?m 131 n?m 133 n?m
CRC (10-8 ?m) 2.65 11.5 12.8 13.1 13.3
LNG (10-8 ?m) 12.8
WEL (10-8 ?m) (293 K-298 K) 12
38 Sr strontium
use 36.4 n?m 123 n?m 132 n?m 134 n?m 135 n?m 222 n?m
CRC (10-8 ?m) 3.64 12.3 13.2 13.4 13.5 22.2
LNG (10-8 ?m) 13.2
WEL (10-8 ?m) (293 K-298 K) 13
39 Y yttrium
use (room temperature) (alpha, polycrystalline) 596 n?m
CRC (10-8 ?m) (290 K-300 K) 59.6
CR2 (10-8 ?m) (room temperature) (alpha, amorphous) 72.5
CR2 (10-8 ?m) (room temperature) (alpha, crystalline) 35.5
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 59.6
LNG (10-8 ?m) 59.6
WEL (10-8 ?m) (293 K-298 K) 56
40 Zr zirconium
use 66.4 n?m 388 n?m 421 n?m 429 n?m 433 n?m 765 n?m
CRC (10-8 ?m) 6.64 38.8 42.1 42.9 43.3 76.5
LNG (10-8 ?m) 42.1
WEL (10-8 ?m) (293 K-298 K) 42
41 Nb niobium
use 152 n?m
CRC (10-8 ?m) 15.2
LNG (10-8 ?m) 15.2
WEL (10-8 ?m) (293 K-298 K) 15
42 Mo molybdenum
use 4.82 n?m 48.5 n?m 53.4 n?m 54.7 n?m 55.2 n?m 106 n?m
CRC (10-8 ?m) 0.482 4.85 5.34 5.47 5.52 10.6
LNG (10-8 ?m) 5.34
WEL (10-8 ?m) (293 K-298 K) 5
43 Tc technetium
use
LNG (10-8 ?m) (100 °C) 22.6
WEL (10-8 ?m) (293 K-298 K) 20
44 Ru ruthenium
use 71 n?m
CRC (10-8 ?m) 7.1
LNG (10-8 ?m) 7.1
WEL (10-8 ?m) (293 K-298 K) 7.1
45 Rh rhodium
use 43.3 n?m
CRC (10-8 ?m) 4.3
LNG (10-8 ?m) 4.33
WEL (10-8 ?m) (293 K-298 K) 4.3
46 Pd palladium
use 17.5 n?m 97.8 n?m 105.4 n?m 107.3 n?m 108.0 n?m 179.4 n?m
CRC (10-8 ?m) 1.75 9.78 10.54 10.73 10.80 17.94
LNG (10-8 ?m) 10.54
WEL (10-8 ?m) (293 K-298 K) 10
47 Ag silver
use 2.89 n?m 14.67 n?m 15.87 n?m 16.17 n?m 16.29 n?m 28.7 n?m
CRC (10-8 ?m) 0.289 1.467 1.587 1.617 1.629 2.87
LNG (10-8 ?m) 1.587
WEL (10-8 ?m) (293 K-298 K) 1.6
48 Cd cadmium
use 68 n?m
use (22 °C) 72.7 n?m
CRC (10-8 ?m) 6.8
LNG (10-8 ?m) (22 °C) 7.27
WEL (10-8 ?m) (293 K-298 K) 7
49 In indium
use 0.080 µ?m 83.7 n?m
CRC (10-8 ?m) 8.0
LNG (10-8 ?m) 8.37
WEL (10-8 ?m) (293 K-298 K) 8
50 Sn tin
use 115 n?m
CRC (10-8 ?m) 11.5
LNG (10-8 ?m) 11.5
WEL (10-8 ?m) (293 K-298 K) 11
51 Sb antimony
use 0.39 µ?m 417 n?m
CRC (10-8 ?m) 39
LNG (10-8 ?m) 41.7
WEL (10-8 ?m) (293 K-298 K) 40
52 Te tellurium
use
LNG (10-8 ?m) (5.8-33)×10³
WEL (10-8 ?m) (293 K-298 K) about 10000
53 I iodine
use 1.3×107 ?m
LNG (10-8 ?m) 1.3×1015
WEL (10-8 ?m) (293 K-298 K) > 1015
55 Cs caesium
use 41.6 n?m 187 n?m 205 n?m 208 n?m 210 n?m
CRC (10-8 ?m) 4.16 18.7 20.5 20.8 21.0
LNG (10-8 ?m) 20.5
WEL (10-8 ?m) (293 K-298 K) 20
56 Ba barium
use 68.3 n?m 302 n?m 332 n?m 0.340 µ?m 343 n?m 724 n?m
CRC (10-8 ?m) 6.83 30.2 33.2 34.0 34.3 72.4
LNG (10-8 ?m) 33.2
WEL (10-8 ?m) (293 K-298 K) 35
57 La lanthanum
use (room temperature) (alpha, polycrystalline) 615 n?m
CRC (10-8 ?m) (290 K-300 K) 61.5
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 61.5
LNG (10-8 ?m) 61.5
WEL (10-8 ?m) (293 K-298 K) 61
58 Ce cerium (beta, hex)
use (room temperature) (beta, polycrystalline) 828 n?m
CRC (10-8 ?m) (beta, hex) (290 K-300 K) 82.8
CR2 (10-8 ?m) (room temperature) (beta, polycrystalline) 82.8
LNG (10-8 ?m) (beta, hex) 82.8
58 Ce cerium (gamma, cubic)
use (room temperature) (gamma, polycrystalline) 744 n?m
CRC (10-8 ?m) 74.4
CR2 (10-8 ?m) (room temperature) (gamma, polycrystalline) 74.4
WEL (10-8 ?m) (293 K-298 K) 74
59 Pr praseodymium
use (room temperature) (alpha, polycrystalline) 0.700 µ?m
CRC (10-8 ?m) (290 K-300 K) 70.0
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 70.0
LNG (10-8 ?m) 70.0
WEL (10-8 ?m) (293 K-298 K) 70
60 Nd neodymium
use (room temperature) (alpha, polycrystalline) 643 n?m
CRC (10-8 ?m) (290 K-300 K) 64.3
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 64.3
LNG (10-8 ?m) 64.3
WEL (10-8 ?m) (293 K-298 K) 64
61 Pm promethium
use (room temperature) estimated 0.75 µ?m
CRC (10-8 ?m) (290 K-300 K) 75 est.
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 75 estimated
LNG (10-8 ?m) 64.0
WEL (10-8 ?m) (293 K-298 K) 75
62 Sm samarium
use (room temperature) (alpha, polycrystalline) 0.940 µ?m
CRC (10-8 ?m) (290 K-300 K) 94.0
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 94.0
LNG (10-8 ?m) 94.0
WEL (10-8 ?m) (293 K-298 K) 94
63 Eu europium
use (room temperature) (polycrystalline) 0.900 µ?m
CRC (10-8 ?m) (290 K-300 K) 90.0
CR2 (10-8 ?m) (room temperature) (polycrystalline) 90.0
LNG (10-8 ?m) 90.0
WEL (10-8 ?m) (293 K-298 K) 90
64 Gd gadolinium
use (room temperature) (alpha, polycrystalline) 1.310 µ?m
CRC (10-8 ?m) (290 K-300 K) 131
CR2 (10-8 ?m) (room temperature) (alpha, amorphous) 135.1
CR2 (10-8 ?m) (room temperature) (alpha, crystalline) 121.7
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 131.0
LNG (10-8 ?m) 131
WEL (10-8 ?m) (293 K-298 K) 130
65 Tb terbium
use (room temperature) (alpha, polycrystalline) 1.150 µ?m
CRC (10-8 ?m) (290 K-300 K) 115
CR2 (10-8 ?m) (room temperature) (alpha, amorphous) 123.5
CR2 (10-8 ?m) (room temperature) (alpha, crystalline) 101.5
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 115.0
LNG (10-8 ?m) 115
WEL (10-8 ?m) (293 K-298 K) 120
66 Dy dysprosium
use (room temperature) (alpha, polycrystalline) 926 n?m
CRC (10-8 ?m) (290 K-300 K) 92.6
CR2 (10-8 ?m) (room temperature) (alpha, amorphous) 111.0
CR2 (10-8 ?m) (room temperature) (alpha, crystalline) 76.6
CR2 (10-8 ?m) (room temperature) (alpha, polycrystalline) 92.6
LNG (10-8 ?m) 92.6
WEL (10-8 ?m) (293 K-298 K) 91
67 Ho holmium
use (room temperature) (polycrystalline) 814 n?m
CRC (10-8 ?m) (290 K-300 K) 81.4
CR2 (10-8 ?m) (room temperature) (amorphous) 101.5
CR2 (10-8 ?m) (room temperature) (crystalline) 60.5
CR2 (10-8 ?m) (room temperature) (polycrystalline) 81.4
LNG (10-8 ?m) 81.4
WEL (10-8 ?m) (293 K-298 K) 94
68 Er erbium
use (room temperature) (polycrystalline) 0.860 µ?m
CRC (10-8 ?m) (290 K-300 K) 86.0
CR2 (10-8 ?m) (room temperature) (amorphous) 94.5
CR2 (10-8 ?m) (room temperature) (crystalline) 60.3
CR2 (10-8 ?m) (room temperature) (polycrystalline) 86.0
LNG (10-8 ?m) 86.0
WEL (10-8 ?m) (293 K-298 K) 86
69 Tm thulium
use (room temperature) (polycrystalline) 676 n?m
CRC (10-8 ?m) (290 K-300 K) 67.6
CR2 (10-8 ?m) (room temperature) (amorphous) 88.0
CR2 (10-8 ?m) (room temperature) (crystalline) 47.2
CR2 (10-8 ?m) (room temperature) (polycrystalline) 67.6
LNG (10-8 ?m) 67.6
WEL (10-8 ?m) (293 K-298 K) 70
70 Yb ytterbium
use (room temperature) (beta, polycrystalline) 0.250 µ?m
CRC (10-8 ?m) (290 K-300 K) 25.0
CR2 (10-8 ?m) (room temperature) (beta, polycrystalline) 25.0
LNG (10-8 ?m) 25
WEL (10-8 ?m) (293 K-298 K) 28
71 Lu lutetium
use (room temperature) (polycrystalline) 582 n?m
CRC (10-8 ?m) (290 K-300 K) 58.2
CR2 (10-8 ?m) (room temperature) (amorphous) 76.6
CR2 (10-8 ?m) (room temperature) (crystalline) 34.7
CR2 (10-8 ?m) (room temperature) (polycrystalline) 58.2
LNG (10-8 ?m) 58.2
WEL (10-8 ?m) (293 K-298 K) 56
72 Hf hafnium
use 67.5 n?m 304 n?m 331 n?m 337 n?m 0.340 µ?m 631 n?m
CRC (10-8 ?m) 6.75 30.4 33.1 33.7 34.0 63.1
LNG (10-8 ?m) 33.1
WEL (10-8 ?m) (293 K-298 K) 30
73 Ta tantalum
use 26.2 n?m 122 n?m 131 n?m 134 n?m 135 n?m 229 n?m
CRC (10-8 ?m) 2.62 12.2 13.1 13.4 13.5 22.9
LNG (10-8 ?m) 13.5
WEL (10-8 ?m) (293 K-298 K) 13
74 W tungsten
use 6.06 n?m 48.2 n?m 52.8 n?m 53.9 n?m 54.4 n?m 103 n?m
CRC (10-8 ?m) 0.606 4.82 5.28 5.39 5.44 10.3
LNG (10-8 ?m) 5.28
WEL (10-8 ?m) (293 K-298 K) 5
75 Re rhenium
use 172 n?m 193 n?m
CRC (10-8 ?m) 17.2
LNG (10-8 ?m) 19.3
WEL (10-8 ?m) (293 K-298 K) 18
76 Os osmium
use 81.2 n?m
CRC (10-8 ?m) 8.1
LNG (10-8 ?m) 8.12
WEL (10-8 ?m) (293 K-298 K) 8.1
77 Ir iridium
use 47 n?m 47.1 n?m
CRC (10-8 ?m) 4.7
LNG (10-8 ?m) 4.71
WEL (10-8 ?m) (293 K-298 K) 4.7
78 Pt platinum
use 19.22 n?m 96 n?m 105 n?m 107 n?m 108 n?m 183 n?m
CRC (10-8 ?m) 1.922 9.6 10.5 10.7 10.8 18.3
LNG (10-8 ?m) 10.6
WEL (10-8 ?m) (293 K-298 K) 10.6
79 Au gold
use 4.81 n?m 20.51 n?m 22.14 n?m 22.55 n?m 22.71 n?m 39.7 n?m
CRC (10-8 ?m) 0.481 2.051 2.214 2.255 2.271 3.97
LNG (10-8 ?m) 2.214
WEL (10-8 ?m) (293 K-298 K) 2.2
80 Hg mercury
use 961 n?m
CRC (10-8 ?m) 96.1
LNG (10-8 ?m) (solid) 21
LNG (10-8 ?m) (liquid) 95.8
WEL (10-8 ?m) (293 K-298 K) 96
81 Tl thallium
use 0.15 µ?m 0.18 µ?m
CRC (10-8 ?m) 15
LNG (10-8 ?m) 18
WEL (10-8 ?m) (293 K-298 K) 15
82 Pb lead
use 49 n?m 192 n?m 208 n?m 211 n?m 213 n?m 383 n?m
CRC (10-8 ?m) 4.9 19.2 20.8 21.1 21.3 38.3
LNG (10-8 ?m) 20.8
WEL (10-8 ?m) (293 K-298 K) 21
83 Bi bismuth
use 1.07 µ?m 1.29 µ?m
CRC (10-8 ?m) 107
LNG (10-8 ?m) 129
WEL (10-8 ?m) (293 K-298 K) 130
84 Po polonium
use (alpha) 0.40 µ?m
CRC (10-8 ?m) 40
LNG (10-8 ?m) (alpha) 40.0
WEL (10-8 ?m) (293 K-298 K) 43
88 Ra radium
use 1 µ?m
LNG (10-8 ?m) 100
WEL (10-8 ?m) (293 K-298 K) 100
90 Th thorium
use 147 n?m
use (22 °C) 15.4
CRC (10-8 ?m) 14.7
LNG (10-8 ?m) (22 °C) 15.4
WEL (10-8 ?m) (293 K-298 K) 15
91 Pa protactinium
use 177 n?m
use (22 °C) 19.1
CRC (10-8 ?m) 17.7
LNG (10-8 ?m) (22 °C) 19.1
WEL (10-8 ?m) (293 K-298 K) 18
92 U uranium
use 0.280 µ?m
CRC (10-8 ?m) 28
LNG (10-8 ?m) 28.0
WEL (10-8 ?m) (293 K-298 K) 28
93 Np neptunium
use (22 °C) 1.220 µ?m
LNG (10-8 ?m) (22 °C) 122.0
WEL (10-8 ?m) (293 K-298 K) 120
94 Pu plutonium
use 1.460 µ?m
LNG (10-8 ?m) 146.0
WEL (10-8 ?m) (293 K-298 K) 150
95 Am americium
use (room temperature) 689 n?m [1]
96 Cm curium
use (room temperature) 1250 n?m [2]
T 80 K (-193 °C) 273 K (0 °C) 293 K (20 °C) 298 K (25 °C) 300 K (27 °C) 500 K (227 °C)

References

  1. ^ The electrical resistivity of 241Am metal. Journal of Physics and Chemistry of Solids Volume 38, Issue 11, 1977, Pages 1301-1305
  2. ^ The electrical resistivity of 244Cm metal. JSolid State Communications Volume 23, Issue 6, August 1977, Pages 389-392

WEL

As quoted at http://www.webelements.com/ from these sources:

  • G.W.C. Kaye and T. H. Laby in Tables of physical and chemical constants, Longman, London, UK, 15th edition, 1993.
  • A.M. James and M.P. Lord in Macmillan's Chemical and Physical Data, Macmillan, London, UK, 1992.
  • D.R. Lide, (ed.) in Chemical Rubber Company handbook of chemistry and physics, CRC Press, Boca Raton, Florida, USA, 79th edition, 1998.
  • J.A. Dean (ed) in Lange's Handbook of Chemistry, McGraw-Hill, New York, USA, 14th edition, 1992.

CRC

As quoted from various sources in an online version of:

  • David R. Lide (ed), CRC Handbook of Chemistry and Physics, 84th Edition. CRC Press. Boca Raton, Florida, 2003; Section 12, Properties of Solids; Electrical Resistivity of Pure Metals

CR2

As quoted in an online version of:

  • David R. Lide (ed), CRC Handbook of Chemistry and Physics, 84th Edition. CRC Press. Boca Raton, Florida, 2003; Section 4, Properties of the Elements and Inorganic Compounds; Physical Properties of the Rare Earth Metals

which further refers to:

  • Beaudry, B. J. and Gschneidner, K.A., Jr., in Handbook on the Physics and Chemistry of Rare Earths, Vol. 1, Gschneidner, K.A., Jr. and Eyring, L., Eds., North-Holland Physics, Amsterdam, 1978, 173.
  • McEwen, K.A., in Handbook on the Physics and Chemistry of Rare Earths, Vol. 1, Gschneidner, K.A., Jr. and Eyring, L., Eds., North-Holland Physics, Amsterdam, 1978, 411.

LNG

As quoted from:

  • J.A. Dean (ed), Lange's Handbook of Chemistry (15th Edition), McGraw-Hill, 1999; Section 4, Table 4.1 Electronic Configuration and Properties of the Elements

See also


  This article uses material from the Wikipedia page available here. It is released under the Creative Commons Attribution-Share-Alike License 3.0.

Electrical_resistivities_of_the_elements_(data_page)
 



 



 
Music Scenes